You’re reading novel Cooley's Cyclopaedia of Practical Receipts Volume I Part 263 online at LightNovelFree.com. Please use the follow button to get notification about the latest chapter next time when you visit LightNovelFree.com. Use F11 button to read novel in full-screen(PC only). Drop by anytime you want to read free – fast – latest novel. It’s great if you could leave a comment, share your opinion about the new chapters, new novel with others on the internet. We’ll do our best to bring you the finest, latest novel everyday. Enjoy!

1. Yellow sand, 20%; kelp, 8%; lixiviated wood-ashes, 30%; fresh wood-ashes, 8%; pale clay, 16%; 'cullet' (broken gla.s.s), 18%. This is the common mixture for coa.r.s.e bottles, in Belgium, France, and Germany.

2. To the last add of black oxide of manganese, 2-1/2 to 3%. Has a rich yellowish colour; used for Rhenish-wine bottles.

3. Pale sand, 51%; lixiviated wood-ashes, 33%; pearl-ashes (dried), 8%; common salt, 7-1/2%; white a.r.s.enic, 1/2%; charcoal, q. s. Very pale green.

4. Siliceous sand (pale), 68-1/2%; potash (or its equiv.), 4%; lime, 23-1/2%; heavy spar, 2-1/2%; peroxide of manganese, 1-1/2%. This forms the celebrated 'flask-gla.s.s' of St. Etienne.

GLa.s.s, BROAD, SPREAD WINDOW GLa.s.s. Sp. gr. 2642.--



_a._ By a.n.a.lysis:--

Silica, 6970%; lime, 1330%; soda, 1525%; oxide of iron (and loss), 175%.

_b._ Materials used:--

1. White sand, 50%; dried sulphate of soda, 22%; charcoal (in powder), 9%; 'cullet,' 41%; peroxide of manganese, a little. Pale.

2. White sand, 60%; potashes (good), 24%; common salt, 10%; nitre, 5%; white a.r.s.enic, 1%; peroxide of manganese, a little (1/12 to 1/10%); pale 'cullet,' at will (10 to 30%). Very pale. This is the 'spread' or 'sheet window-gla.s.s' in common use.

GLa.s.s, CHEMICAL. Sp. gr. 2390 to 2396.--

_a._ By a.n.a.lysis:--

1. Silica, 7280%; pota.s.sa, 1680%; lime (with a trace of alumina), 968%; magnesia, 40%; traces of oxide of manganese and iron (and loss) 32%. This is the difficultly fusible 'Bohemian tube-gla.s.s,' so valuable in chemical manipulations.

2. Silica, 693%; pota.s.sa, 158%; soda, 3%; lime, 76%; alumina, 12%; magnesia, 2%; oxide of iron, 5%; oxide of manganese (and loss), 6%.

English chemical gla.s.s (without lead). More fusible than the last.

_b._ Materials used:--

1. Quartz (hyalin, in powder), 60%; calcined purified pearlash, 30%; fresh-burnt lime (very pure), 9%; nitre (dried), 3/4%; a.r.s.enious acid or peroxide of manganese, 1/4%. Said to be the proportions used in the production of _a_, 1 (_above_).

2. (M. Peligot.) Quartz, 71-1/2%; carbonate of pota.s.sa (or its equiv., dry), 20%; quicklime, 8-1/2%; (manganese, a little). Said to be the formula for the hardest and least fusible 'Bohemian tube-gla.s.s.' It is very intractable and infusible, except at a very high temperature; but the addition of an exceedingly small quant.i.ty of boracic acid, borax, or a.r.s.enious acid, causes it to flow into a gla.s.s possessing great brilliancy and hardness, and capable of being wrought at the highest heat of the ordinary furnace.

GLa.s.s, CROWN, WHITE WINDOW-GLa.s.s. Sp. gr. 2486 to 2488.--

_a._ By a.n.a.lysis:--

1. Silica, 628%; pota.s.sa, 221%; lime, 155%; alumina (with traces of oxide of iron and manganese), 26%. Crown-gla.s.s of Bohemia, according to Dumas. Very beautiful.

2. Silica, 725%; soda, 1775%; lime, 975%. English crown-gla.s.s; excellent quality, but not so white as the last.

_b._ Materials used:--

1. Finest white siliceous sand, 64%; purified potashes (dry), 23%; lime, 12%; white a.r.s.enic, 3/4%; oxide of manganese, 1/4%. Said to be used in Bohemia.

2. (Schweigger.) Pure sand, 57%; dry sulphate of soda, 28-1/2%; quicklime, 11-1/2%; powdered charcoal, 3 or 4%. Corresponds to _a_, 2, _above_ (nearly).

3. Pure sand, 40%; soda ash, 24%; lime, 5%; white 'cullet,' 31%, Rather superior to the last.

CRYSTAL, CRYSTAL GLa.s.s. The 'crystal gla.s.s' of England is flint gla.s.s' of superior quality; that of Bohemia is noticed under TABLE GLa.s.s.

GLa.s.s, FLINT, CRYSTAL. Sp. gr. 3000 to 3620.--

_a._ By a.n.a.lysis:--

1. (Berthier.) Silica, 5919%; oxide of lead, 2868%; pota.s.sa, 1213%; oxides of iron and manganese, traces. Finest colourless English crystal.

2. (Brande; Faraday.) Silica, 52%; oxide of lead, 34%; pota.s.sa, 34%.

Crystal.

3. (Faraday.) Silica, 4430%; oxide of lead, 4305%; pota.s.sa, 1175%; alumina, 50%; oxides of iron and manganese, 12%; (loss 28%). Heaviest of three samples of flint gla.s.s examined.

_b._ Materials used:--

1. Finest Lynn-sand (calcined, sifted, and washed), 51%; litharge (purest), 28% (or red lead, 29%), refined pearlashes (calcined before being weighed), 16%; nitre (purified), 4-3/4% a.r.s.enious acid and peroxide of manganese, of each, 1/8%. Very fine crystal.

2. (M. Payen.) Fine sand, 46%; red lead, 31%; purified carbonate of potash, 23%. French crystal.

3. (Geddes.) White Lynn-sand, 51%; red lead or litharge, 33%; refined pearlashes, 13%; nitre, 3%; a very little a.r.s.enious acid and peroxide of manganese. Ordinary English flint-gla.s.s. Crystal 'cullet' may be added at will to the above. This gla.s.s was originally prepared from powdered flints, a fact to which it owes its common name.

GLa.s.s, OPTICAL. 1. (Crown gla.s.s.) Purest siliceous sand, 55%; carbonate of soda (dry), 12%; chalk (dry), 11%; carbonate of baryta, 22%.

2. (Flint gla.s.s.)--

_a._ By a.n.a.lysis:--

Silica, 4430%; oxide of lead, 4305%; pota.s.sa, 1175%. This is Guinand's 'dense optical gla.s.s.'

_b._ Materials used:--

1. Purest quartz, 42%; red lead (finest), 42%; purified potash, 14-3/4%; purified nitre, 1-1/4%. These are the proportions used for the last.

2. (Korner.) Finest quartz (reduced to powder, treated with hydrochloric acid, washed, and dried), 47-1/2%; red lead, 38-1/4%; cream of tartar, 14-1/2%. The above are used by opticians in the construction of achromatic object-gla.s.ses.

GLa.s.s, PLATE. Sp. gr. 2488 to 2600.--

_a._ By a.n.a.lysis:--

1. (Dumas.) Silica, 759%; soda, 175%; lime, 38%; alumina, 28%. French mirror-gla.s.s.

2. (Mitscherlich.) Silica, 60%; pota.s.sa, 25%; lime, 125%; loss, 25%(?).

Finest Bohemian plate.

_b._ Materials used:--

1. Finest siliceous sand, 45%; dried carbonate of soda, 25%; lime, 5%; nitre (purified), 2%; plate-gla.s.s cullet, 23%; peroxide of manganese and cobalt azure, a very little. Ordinary English plate.

2. Whitish quartz sand, 60%; purified carbonate of soda (dried), 20%; lime (slaked by exposure to the air), 9%; plate-gla.s.s cullet, 11% (or more).

Cooley's Cyclopaedia of Practical Receipts Volume I Part 263

You're reading novel Cooley's Cyclopaedia of Practical Receipts Volume I Part 263 online at LightNovelFree.com. You can use the follow function to bookmark your favorite novel ( Only for registered users ). If you find any errors ( broken links, can't load photos, etc.. ), Please let us know so we can fix it as soon as possible. And when you start a conversation or debate about a certain topic with other people, please do not offend them just because you don't like their opinions.


Cooley's Cyclopaedia of Practical Receipts Volume I Part 263 summary

You're reading Cooley's Cyclopaedia of Practical Receipts Volume I Part 263. This novel has been translated by Updating. Author: Arnold Cooley and Richard Tuson already has 750 views.

It's great if you read and follow any novel on our website. We promise you that we'll bring you the latest, hottest novel everyday and FREE.

LightNovelFree.com is a most smartest website for reading novel online, it can automatic resize images to fit your pc screen, even on your mobile. Experience now by using your smartphone and access to LightNovelFree.com

RECENTLY UPDATED NOVEL